Friday, April 18, 2025

[MW:35536] RANGE ASME SEC IX

Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.

Re: [MW:35537] RANGE ASME SEC IX

What is the diameter of the pipe to be welded , ASME IX give a limit on the diameter to be welded by a welder that has been qualified in a plate and what positions they can weld 

On Wed, 16 Apr 2025 at 08:57, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.


--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT_qMzt7TESHXC2-%3DM3_7gmsbCznt5h4MhkxwYu7-GzNtg%40mail.gmail.com.

Re: [MW:35538] RANGE ASME SEC IX

PIPE DIA :24 INCH AND 26 INCH 
We have WQT for 2G & 3 G position 
Production weld 1G FLAT POSITION 




On Wed, 16 Apr 2025 at 12:17 PM Rilley Chellah Mulenga <rilley.mulenga@ahkgroup.com> wrote:
What is the diameter of the pipe to be welded , ASME IX give a limit on the diameter to be welded by a welder that has been qualified in a plate and what positions they can weld 

On Wed, 16 Apr 2025 at 08:57, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.


--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT_qMzt7TESHXC2-%3DM3_7gmsbCznt5h4MhkxwYu7-GzNtg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ym18YD40u%2BVCKGryzERQUW6jKwaXZkOTxmECjG%3Dv6WXnw%40mail.gmail.com.

Re: [MW:35539] RANGE ASME SEC IX

For WPS/PQR qualification, Diameter is an non essential variable according to ASME Sec.IX and position is a supplementary essential variable and only progression UP or DOWN counts.

For Welder Qualification check QW-461.9 Table & Table QW-452.3

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



On Wednesday 16 April, 2025 at 01:47:36 pm IST, Rilley Chellah Mulenga <rilley.mulenga@ahkgroup.com> wrote:


What is the diameter of the pipe to be welded , ASME IX give a limit on the diameter to be welded by a welder that has been qualified in a plate and what positions they can weld 

On Wed, 16 Apr 2025 at 08:57, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.


--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT_qMzt7TESHXC2-%3DM3_7gmsbCznt5h4MhkxwYu7-GzNtg%40mail.gmail.com.

Re: [MW:35540] RANGE ASME SEC IX

  Dear Mr. Elavarasan,
  Plate to Pipe Qualification: A welder qualified on a plate is qualified to weld on pipe, but there are diameter and position restrictions
  Pipes of OD 24 and 26 inches, are well above 73 mm, so diameter is not a restricting factor for your case.
  For your 25 mm plate: The qual. range is 12.5 to 50 mm for production welds (with impact testing).
  24-inch pipe (9.5 mm wall):    Not qualified, as the wall thickness is less than the minimum qualified thickness of 12.5 mm.
  26-inch pipe (14 mm wall) :    Qualified, as the wall thickness is within the qualified range.
  8 mm wall thickness pipe:       Not qualified, as it is below the minimum qualified thickness.
  Welder Qualification (WQT): The same thickness rules apply to the welder as to the procedure, unless the welder was qualified
                                                   on pipe directly, in which case the thickness and diameter ranges may differ.
                                                                                  If you need to weld pipes with wall thickness less than 12.5 mm (such as 8 mm or 9.5 mm), you must                   
                                                   requalify the procedure and welder for that thickness range.
  Conclusion:
  • You cannot use the current plate WPS and WQT to weld a 24-inch pipe with 9.5 mm wall thickness or any pipe with 8 mm wall thickness.

  • You can use them for a 26-inch pipe with 14 mm wall thickness.

  • To weld thinner pipes (8 mm, 9.5 mm), you must qualify a new WPS and WQT for those thicknesses.

   Both 9.5 mm and 14 mm pipes generally require impact testing (as per ASTM A333/A333M-15 and other standards, especially    

   if impact properties are specified in the material grade or project specifications specify impact toughness as a mandatory property. 


   References:

   ASME Section IX, Table QW-451.1 and QW-452 

   Welder qualification diameter and thickness ranges.                                                                                                                                                                                                                                  

                                                                                                                                                                                                                                                                                                                                                                                                         Hope it is clear

   rgds,

   C Sridhar.

   -------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


 


   





On Wed, 16 Apr 2025 at 12:27, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiyL0rY6PzhtTQCT2u-HKR_vXqisFY3JyQNuSRVnZwL2A%40mail.gmail.com.

Re: [MW:35541] RANGE ASME SEC IX

Dear Sridhar 
                       In my case we have qualified WPS with impact requirement 
WPS 1.  BASE PLATE THICKNESS 8 mm 
WPS 2. BASE PLATE THICKNESS 25 mm
QUALIFIED WQT : 25 mm PLATE  

 Welder qualifications need to be consider impact requirement or not as per ASME sec IX 
  
Above mentioned 25 mm thick base plate WQT.    can use  production weld ( 8mm to 25mm) please clarify 

ELAVARASAN


On Wed, 16 Apr 2025 at 2:33 PM sridhar cn <sridharcn305@gmail.com> wrote:
  Dear Mr. Elavarasan,
  Plate to Pipe Qualification: A welder qualified on a plate is qualified to weld on pipe, but there are diameter and position restrictions
  Pipes of OD 24 and 26 inches, are well above 73 mm, so diameter is not a restricting factor for your case.
  For your 25 mm plate: The qual. range is 12.5 to 50 mm for production welds (with impact testing).
  24-inch pipe (9.5 mm wall):    Not qualified, as the wall thickness is less than the minimum qualified thickness of 12.5 mm.
  26-inch pipe (14 mm wall) :    Qualified, as the wall thickness is within the qualified range.
  8 mm wall thickness pipe:       Not qualified, as it is below the minimum qualified thickness.
  Welder Qualification (WQT): The same thickness rules apply to the welder as to the procedure, unless the welder was qualified
                                                   on pipe directly, in which case the thickness and diameter ranges may differ.
                                                                                  If you need to weld pipes with wall thickness less than 12.5 mm (such as 8 mm or 9.5 mm), you must                   
                                                   requalify the procedure and welder for that thickness range.
  Conclusion:
  • You cannot use the current plate WPS and WQT to weld a 24-inch pipe with 9.5 mm wall thickness or any pipe with 8 mm wall thickness.

  • You can use them for a 26-inch pipe with 14 mm wall thickness.

  • To weld thinner pipes (8 mm, 9.5 mm), you must qualify a new WPS and WQT for those thicknesses.

   Both 9.5 mm and 14 mm pipes generally require impact testing (as per ASTM A333/A333M-15 and other standards, especially    

   if impact properties are specified in the material grade or project specifications specify impact toughness as a mandatory property. 


   References:

   ASME Section IX, Table QW-451.1 and QW-452 

   Welder qualification diameter and thickness ranges.                                                                                                                                                                                                                                  

                                                                                                                                                                                                                                                                                                                                                                                                         Hope it is clear

   rgds,

   C Sridhar.

   -------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


 


   





On Wed, 16 Apr 2025 at 12:27, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiyL0rY6PzhtTQCT2u-HKR_vXqisFY3JyQNuSRVnZwL2A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ykQRXOuc5SuKydUyUHpRFKXawrOjQEcg5TK6ZJvJWJ4vg%40mail.gmail.com.

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...