Thursday, July 16, 2020

Re: [MW:31149] CS with Duplex SS (S31803) clad vessel PWHT?

no problem boss go for it today i did the same no problm i did mpt from outside of vessel after pwht and lpt from inside at weld ,check fe number no problem

On Sun, 12 Jul 2020, 6:54 pm Customer Care, <bricenori@hotmail.com> wrote:

Hi,

You can realize the dissimilar welding (CS 516 Gr.70) + Cladding (S31803) with PWHT following these steps:

-As the base metal of CS have 51 mm of thickness, apply preheating about 175 °C and maintain it during the welding.   Use filler for CS type E/7018 (depending welding process).

 

-Buttering the CS with austenitic filler metal (e.g., E/309L) and remove clad S31803 with grinding, 2" side and side of the weld joint. Realize localized PWHT over the weld metal and HAZ only, about 625 °C during one and half hours.

             - Weld the S31803 clad using duplex filler like E/2209.

 

Ramon Briceno

Senior Metallurgical Engineer / Oil & Gas

 

 

Sent from Mail for Windows 10

 

From: Materials & Welding
Sent: Saturday, July 11, 2020 6:42 AM
To: Materials & Welding
Subject: [MW:31131] CS with Duplex SS (S31803) clad vessel PWHT?

 

ASME Sec VIII div1

SA516 Gr 70 - 51mm thickness+S31803 clad

 

any experience on duplex clad vessel PWHT?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d1dd74b8-9481-47ce-a896-8d41a29c527cn%40googlegroups.com.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BL0PR03MB42430F71AF631FA12E6C9631AA630%40BL0PR03MB4243.namprd03.prod.outlook.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOWr6k_5BwAM6%2Bgof_z7wr7tw%3DOu5MH9WhVpps_8xdwzm6_juw%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...