Hi  ASN,

 

MR 103 clearly specifies under scope: The materials, heat treatments, and material property requirements set forth in NACE MR0103 are based on extensive experience in the oil and gas production industry, as documented in NACE MR0175/ISO 15156, and were deemed relevant to the refining industry by the MR-103 task group.

 

In order to qualify SS 321H for MR-103 : It  shall meet the chemical composition requirements specified in Table-3., shall not exceed 22 HRC, shall be in the solution-annealed and quenched or solution-annealed and thermally stabilized condition, and shall be free of cold work intended to enhance their mechanical properties. Austenitic stainless steels containing lead or selenium for the purpose of improving machinability are not allowed.

 

Table 3 - Chemical composition requirements for austenitic stainless steels

Element Mass percentage.

C 0,10 max

Cr 16,0 min

Ni 8,0min

Mn 2,0 max

Si 2,0 max

p 0,045 max

s 0,04 max

·         Unlisted elements, such as molybdenum, nitrogen, titanium, and niobium (columbium), are allowed provided that the chemical composition requirements in Table 3 are met.

 

As stated above many of the materials adopted by MR-0103 were based on the extensive "Qualification, Acceptance and in Service Experience Regime" of MR-0175/ISO15156.

 

Hence it's not mandatory for the OEM to Stamp or Etch Mark on the Component as Products being in conformance to MR-0103.If client strongly insists on this point it may be a matter of agreements between the OEM (Supplier) and the End User (Client). However compliance statements on the materials certificates (MTR) is mandatory , when the technical requirements of MR-0103 (as stated above ) are fulfilled.

 

Based on the facts provided below, I would say supplier is on the right track.

 

Hope this clarifies your query.

 

Thanks.

 

 

P.Goswami.P.Eng, IWE.

Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of SRINI
Sent: December 13, 2017 11:52 AM
To: materials-welding@googlegroups.com
Subject: [MW:27188] MR0103 Marking required or LOC . Which one acceptable

 

Dear Sir,

 

Material: ASTM 182 Gr 321H (FLANGE)

Size:1/2 inch x sch 80 s

 

As per client requirement MR0103

Manufacture not marking on flange as MR0103 , But manufacture given LOC for flange as meeting requirement MR0103.

 In MR0103 did not mentioned formarking,but MR0175 they mentioned at para 7.1 marking or documents also acceptable.

 

1)Is it acceptable or not.

2) according to which standard.

 

Please give advice and solution.

 

Regards

ASN

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


Virus-free. www.avg.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...