Tightening torques for stainless steel bolts

Introduction

Minimum breaking torque (M b,min) for austenitic grade bolts and screws between M 1.6 and M 16 (course threads) are shown in table 4 of BSENISO 3506-1:1997. This shows torque values in Nm for property classes 50, 70 and 80 as shown in the table below. This applies to 'grades' A1, A2, A3, A4 and A5. Tightening torque values are not given in this standard.

Minimum breaking torque values

Torque values are not given for martensitic (C1, C3, C4) or ferritic (F1) grades. The standard states that these values are to be agreed between manufacturer and user.

 

Min breaking torque Nm for property class

 

50

70

80

M1.6

0.15

0.2

0.24

M2

0.3

0.4

0.48

M2.5

0.6

0.9

0.96

M3

1.1

1.6

1.8

M4

2.7

3.8

4.3

M5

5.5

7.8

8.8

M6

9.3

13

15

M8

23

32

37

M10

46

65

74

M12

80

110

130

M16

210

290

330

 

Maximum tightening torque, yield loads and failure loads for austenitic stainless steel fasteners

Tightening torques, yield loads and failure loads are not given in the BSENISO 3506-1:1997 standard. Some data is available however on the Bufab UK web site.

 

Source: http://www.bssa.org.uk/

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...