Hello, This information is very usefull.

Currently I have a requirement to produce M8 --8.8 grade Bolt. 
Can I select material C40 for the same.

Ajith

On Friday, December 7, 2012 at 5:15:19 PM UTC+5:30, scb wrote:

Mr.Bhaskar,

 

This is fastener standard for bolts

Grade 8.8 means , Approx. 800 MPa TS and 640 MPa yield strength(  you will arrive at the YS by multiplying the both the numbers times 10. That is 8x8x10=640)

Similarly  , 10.9 means  approx.1000 MPa  TS and 900 MPa yield strength. I have given below the exact details.

 

 

Property Class

Tensile strength,Mpa

Hardness

Material

heat treatment

tempering

4.6

400

B67-B87

low or medium carbon steel witth max limits for C 0.55, P0.048, S0.058

no

 

4.8

420

B71-B87

5.8

520

B82-B95

8.8

830

C23-C34

 medium carbon steel with max limits for C0.28- 0.55, P0.048, S0.058

oil quenched

 min 425 deg C

9.8

900

C27-C36

 min 410 deg C

10.9

1040

C33-C39

 min425  deg C

12.9

1220

C38-C44

 medium carbon steel with max limits for C0.31- 0.65, P 0.045 MAX, S 0.045MAX

oil quenched

min 380deg C

 

I hope this will clarify your point. If any questions please don't hesitate to write.

 

Regards,

 

S C Balawat.

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of v baskar
Sent: Friday, December 07, 2012 3:01 PM
To: material...@googlegroups.com
Subject: [MW:16160] Difference between IS 1367 Gr. 4.6, 8.8 & 10.9

 

Dear Members,

 

I would like to know difference between IS 1367 Gr. 4.6, 8.8 & 10.9

What does "4.6", 8.8 and "10.9" means....... 

 

Thankyou

 

V. B.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/446d60dc-1874-4d29-8cb2-54ecaac10e2a%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...