Re: [MW:14984] Stress relieving of 410S

which electrode are u using for this purpose..i think it'z not
E309..if u r using E 410-XX electrode for welding, then heat to
730-760°C and hold for one hour before cooling it to ambient
temperature.. Refer SFA 5.4 Table 6..

On 7/28/12, kundan.ahirao@gmail.com <kundan.ahirao@gmail.com> wrote:
> Dear expert
> kindly advice and share your opinion
> we have cladding of SA516 gr 70 + SA 240 tp 410S.
> After explosion bonding manufacturer is giving SR cycle to clad plate at
> soaking temp 675 deg C.
> But at this temperature tensile strength of base metal will achieve or not.
> If not then what will be soaking temperature.
> Also as per our fabrication drg soaking temp given is 620 deg C.
> Thanks and regards
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...