We have to intrepret as follows.
 
a. No single unbonded area should not exceed 58 cm2
b. Even if the unbonded area is less than 58cm2 the unbonded area not to exceed 5% of the total claded suface area(in my opinion we may bound t happend this in small size plates)
 
br,
 
msms
On Sun, Jul 22, 2012 at 10:30 AM, <kundan.ahirao@gmail.com> wrote:
Dear Expert
please advice-----
Recently we received some explosion bonded clad plate of SA516 gr 70 + SA 240 Tp 316L.
During explosion bonding plate having unbonded area.
As per SA 264 cl No 13.3.3 says that no single unbonded area exceeding 58cm2 with total unbonded area not to exceed 5% of the total cladded surface area.
Does it mean that above 58cm2 unbonded area are not acceptable or above 58cm2 unbonded area repairable upto 5% of total cladded surface area.

Thanks and Regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...