Re: [MW:14424] SS347 overlay but FN is too low

Lower the Amperage, Higher the velocity.


Roy
Bohler Welding Group


-----原始邮件-----
From: bo gyi
Sent: Thursday, May 31, 2012 8:40 AM
To: Materials & Welding
Subject: [MW:14422] SS347 overlay but FN is too low

Dear all,

I have encountered that Ferrite No is too low for SS347 overlay to P1
(SAW).

I used ESAB ER309L & ER347 together with OK flux 10.93 and heat input
is about 0.9 - 1 kJ/mm.

My Ferrite no is as bellow . (check by Ferrite scope)

1st layer 309L (2mm thk from BM) , FN no. < 0.5

2nd layer 347 ( 4 mm thk from BM) , FN no < 2

3rd layer 347 ( 6 mm thk from BM) , FN no < 3.5

Required FN is 5 to 11 FN,

My welding parameters are as follow.

For 309L , 280 � 330 A, 30 � 32 V , travel speed 720 � 800 mm/min

For 347 , 330 � 350 A, 32 � 34 V , travel speed 720 � 800 mm/min


Please advice.

Regards,

Bogyi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...