Dear
Red hot tendency could occur.
1) If you are using higher currents than the required one. In general 40Amps
per dia is the amperage followed. Being Stainless Steel electrode, 80-90
Amps for 2.5mm dia can be used.
2) Could be due to Eccentricity. While manufacturing process during
extrusion, if the flux is not quoted uniformly on the core wire, then also
this problem could happen. It is normally a batch problem.
You can try either.
1) Use lesser currents. You have not mentioned the currents kept during
welding.
2) Try different batch of electrodes.
Regards
Fredric Prabu. K
-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
murtaza506@yahoo.com
Sent: Tuesday, May 29, 2012 5:34 PM
To: Materials & Welding
Subject: [MW:14386] MMA welding Electrode Gets red hot
I have a MMA welding electrode of SS 308L Dia. 2.6mm. when half of the
electrode is consumed it get red hot, and it gives porosity in the weld
metal what could be the reason i.e. is it a welding problem or there is a
problem in the electrode???
if this problem is due to electrode then what can be the reasons and
rectifications???
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment