Dear all,
I have encountered that Ferrite No is too low for SS347 overlay to P1
(SAW).
I used ESAB ER309L & ER347 together with OK flux 10.93 and heat input
is about 0.9 - 1 kJ/mm.
My Ferrite no is as bellow . (check by Ferrite scope)
1st layer 309L (2mm thk from BM) , FN no. < 0.5
2nd layer 347 ( 4 mm thk from BM) , FN no < 2
3rd layer 347 ( 6 mm thk from BM) , FN no < 3.5
Required FN is 5 to 11 FN,
My welding parameters are as follow.
For 309L , 280 – 330 A, 30 – 32 V , travel speed 720 – 800 mm/min
For 347 , 330 – 350 A, 32 – 34 V , travel speed 720 – 800 mm/min
Please advice.
Regards,
Bogyi
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Subscribe to:
Post Comments (Atom)
[MW:35668] Selection of Filler/Electrode.
Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment