Re: [MW:14036] Heat input value in WPS

Thank u TG
 Can u give the detail example so that i can understood more.

Nilesh

On Fri, Mar 30, 2012 at 2:25 PM, Tarantula Ghosh <ghosh.tarantula@gmail.com> wrote:
Hi Nilesh,
'matter of fact the lower range value is equally important. If the heat input is reduced as compared to PQR values, tendency to harden increases as cooling rate is increased. In your WPS, you need to mention the range as recorded in the PQR.
TG


On Fri, Mar 23, 2012 at 11:53 AM, Prashant Shelar <pshelar@lamprell.com> wrote:

Hi Nilesh,

 

Being impact as a requirement, you will have to limit the maximum Heat Input value in WPS as qualified in the PQR. You will have to indicate the values on WPS with upper limit restricted to that in PQR.

 

Thanking you,

Rgds,

 

Prashant

 

 

 

 

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of waman nilesh
Sent: Friday, March 23, 2012 11:07 AM
To: materials-welding@googlegroups.com; materials-welding@goolegroups.com
Cc: wamannp@yahoo.com
Subject: [MW:13977] Heat input value in WPS

 

Dear Experts,

I have question we are doing WPS, PQR & WPQ ( Material- IS 2062 GR B & thickness- 20 mm ) as per EN 15614 standard in which impact is essential.

So which value of heat input is to be mention on  WPS.

 

With Regards,

Nilesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



Any views or opinions expressed in this email and its attachments are those of the individual sender except where the sender specifically states them to be that of Lamprell.

This E-mail and any attachments are confidential and may also be legally privileged. If you have received this email and any attachments in error, you are on notice of its status. Please (a) notify the sender immediately by reply email; (b) destroy this email and any attachment, and (c) do not use, copy, store and/or disclose to any person this email and any attachments: to do so could be a breach of confidence. Thank you for your co operation. Please contact the Lamprell IT Helpdesk on ithelpdesk@lamprell.com if you need any assistance.

Holding company: Lamprell plc, incorporated in the Isle of Man, registration number 117101C, registered office at Fort Anne, Douglas, Isle of Man IM1 5PD

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Tarantula



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...