Hi Harish
 
For welding 13-14% Mn Steels you can use Austenitic manganese steel : E18-8-6 type SMAW electrodes or FCAW wires.
This electrode contains 0.1-0.4%C, 18%Cr, 8%Ni and 6% Mn. The weld deposits are work hardenable type. As deposited hardness=200HB, after workhardening= 47 HRC.
Welding has to be done very slowly with controlled interpass temp. of 150 degrees Celcius max.
Mostly the component is immersed in a water bath tub during welding to maintain the interpass temp.
Also weld with low heat input, lower current settings. Weld stringer and short beads.
 
If you tell me the application i can give you the solution as i have welded plenty of Hadfield steels !
 
Regards
 
Prem Nautiyal 
Cell: 9004063879 / 9769316004
 
From: Harish Kannepalli <harishkannepalli@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, April 18, 2012 10:19 PM
Subject: [MW:14124] 13% Mn steel Welding

Dear Experts,
                     Please share some welding data on 13% Mn (Hadfield) steel. Like electrode, suppliers, welding parameters.


regards,
Harish.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...