Dear Vaibhav:

My suggestions are as per following:
  1. Go with E310 type electrode.
  2. Use techniques which result in less dilution of the weld metal (by CS and 410).
  3. A 150-250 Deg preheat is recommended to avoid cracking of 410 (higher temp for higher thickness).
  4. Maintain minimum of 150 Deg inter-pass temperature.
  5. Apply PWHT to temper HAZ of 410 base metal (between 650-700 Deg for minimum of 30 minutes).
Good Luck
Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
  


On Tue, Apr 3, 2012 at 1:40 PM, vpuranik <vpuranik@deltechcontrols.com> wrote:

Dear experts,

 

Please suggest the welding procedure and welding parameters to weld WCB body and SS 410 Ring and also suggest welding electrode for welding.

 

 

Thanks & Regards.

 

Vaibhav V Puranik.

(Manufacturing Engineer)

 

Delval Flow Controls (P) Ltd.

Gat.No.625 /1/2,Kuruli,3

Tal Khed,Pune-Nashik Highway,

Pune-410501,India

Phone:02135-662700 / 662716.  Fax: 02135-662727

Cell:+91 8308829850 Email: vpuranik@deltechcontrols.com

I could not wait for success, so i went ahead without it.

 

 

 

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...