Re: [MW:14080] suggest the welding procedure to weld WCB with SS 410 ring

Hi Vaibhav
 
I have done similar job in past with ER309L and E309L.
Preheat upto min. 200 degrees C.
No PWHT is required as you are welding with austenitic filler E309L.
 
As per customer technical specs. we had also done micro examination at 200X mag. in PQR, inorder to check internal micro cracks and the result was satisfactory.
This is a proven method and can be followed in your PQR.
 
Please drop a line if you have any further doubts.
 
Regards
 
Prem Nautiyal
Mobile     +91-9004063879 / 9769316004


--- On Fri, 4/6/12, Ramin Kondori <raminkondori@gmail.com> wrote:

From: Ramin Kondori <raminkondori@gmail.com>
Subject: Re: [MW:14079] suggest the welding procedure to weld WCB with SS 410 ring
To: materials-welding@googlegroups.com
Date: Friday, April 6, 2012, 11:59 PM

Dear Vaibhav:

My suggestions are as per following:
  1. Go with E310 type electrode.
  2. Use techniques which result in less dilution of the weld metal (by CS and 410).
  3. A 150-250 Deg preheat is recommended to avoid cracking of 410 (higher temp for higher thickness).
  4. Maintain minimum of 150 Deg inter-pass temperature.
  5. Apply PWHT to temper HAZ of 410 base metal (between 650-700 Deg for minimum of 30 minutes).
Good Luck
Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
  


On Tue, Apr 3, 2012 at 1:40 PM, vpuranik <vpuranik@deltechcontrols.com> wrote:

Dear experts,

 

Please suggest the welding procedure and welding parameters to weld WCB body and SS 410 Ring and also suggest welding electrode for welding.

 

 

Thanks & Regards.

 

Vaibhav V Puranik.

(Manufacturing Engineer)

 

Delval Flow Controls (P) Ltd.

Gat.No.625 /1/2,Kuruli,3

Tal Khed,Pune-Nashik Highway,

Pune-410501,India

Phone:02135-662700 / 662716.  Fax: 02135-662727

Cell:+91 8308829850 Email: vpuranik@deltechcontrols.com

I could not wait for success, so i went ahead without it.

 

 

 

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...