Dear Mr P.Goswami
 
We are using only ASME B 31.1 & IBR codes for general pipe bends, we are not refering specifically for Induction bending.
 
Bend pipe details:
SA 335 P22, Φ660x44mm,
 ROB-991mm, DOB-90°,
 Intrados temperature-1050°C,
Extrados temperature-990°C,
 Quench type-Air quench.
 
Hardness shall be around 200 Hv
 
Pandithan
 

On Mon, Jul 4, 2011 at 3:58 PM, pgoswami <pgoswami@quickclic.net> wrote:
What's the induction bending code you're following? What's the pipe wall thickness? Is there any hardness restriction the bends?
 
Appreciate your feedback.
 
Thanks.
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of kannayeram gnanapandithan
Sent: Sunday, July 03, 2011 11:16 AM
To: materials-welding@googlegroups.com
Subject: [MW:11583] PBHT FOR SA335GrP22

DEAR EXPERTS
                      IS IT REQUIRED  TO DO PBHT FOR P22 MATERIAL WHICH WAS BENT IN INCREMENTAL HOT INDUCTION PIPE BENDING WITH TEMP 990 DEGRE CELSIUS WITH AIR QUENCHING
 
PANDITHAN
IN-CHARGE/WELDING TECH
CETHAR LIMITED
TRICHY 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...