[MW:5797] RE: 5792] FW: 5772- ASTM G 48 testing for SDSS

Dear Sudhakar,

 

In addition to the restriction mentioned in the trailing mail, control on heat input is more critical in Super DSS materials such as UNS S32750. Based on my previous experience on these materials, I would suggest heat input limit should be 1- 1.5 Kj/mm for smaller thickness and 2 Kj/mm max for thicker sections.

 

As Mr. Goswami suggested, the ferrite to austenite ratio also critical for G 48 testing. Heat input increases, the rate of cooling would be reduced, and in tern more % of ferrite formation in the final weld. It means that we are allowing more time to transform austenite to ferrite when we use increased heat input. In general the % of ferrite in the weld should be 35 – 65%.

 

Using lower heat input would minimize the formation of ferrite which is more important for SDSS welds.

 

Regards,

 

L. Prabhu kumar,


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Wednesday, June 30, 2010 6:42 AM
To: materials-welding@googlegroups.com
Subject: [MW:5792] FW: 5772- ASTM G 48 testing for SDSS

 

 

Dear Sudhakar,

 

ASTM G48A(72 hrs), or and modified versions(24 hrs) is the most common specified corrosion test for duplex or super duplex S.S. This test is considered to be a check of the metallurgical condition of the steel rather than  its performance in any service environment.  The ferric chloride solution is very aggressive and resembles actual industrial service environments.

 

For base metals specified test temperatures vary considerably and are 22.5–30°C for 22Cr duplex and 35–60°C for 25Cr duplex(A790, S32750). In ASTM G48A, 72hour test period is stipulated, however shorter version  24hour  exposure is also used  in the industry.

 

For 22Cr duplex, the experience from service as well as from testing according to various specifications is extensive and shows that a test temperature of 22.5–25°C is suitable to ensure that materials properties after welding and heat treatment operations are within the limits expected for 22Cr duplex.

 

For 25Cr duplex, a combination of laboratory test results and service experience, although not as extensive as for 22Cr duplex, strongly indicate that   50°C is a suitable test temperature for solution annealed base metal products.

 

For welded coupons of 32750 typical recommendations of testing temperature of 400C , and either 24 or 72 hrs of exposure time, with no pitting  be present  20X magnification.

 

From my past experiences in such materials I could advise you on these aspects:-

 

Ā·         Choose the base metal and weld filler metal with ASTM G48A  or G48 C (determination of CPT)  test done typically @ 50°C

Ā·         Monitor welding parameters closely, and stick to the welding heat input of 2-3 KJ/mm criteria. Super Duplex 32750 have a tendency to form excess ferrite, which may to turn to sigma phase, for thick section welding. Composition of shielding and backing gas(Argon+ Nitrogen) would be critical.

Ā·         I presume that  ASTM G-48A test is not the only test you’re going to perform. If not look out for the test results of Ferrite count test, a good ferrite to austenite ratio  and relative absence of sigma phase could be a good way to start for corrosion test.

Ā·         Surface preparation of samples could affect the test results. Generally after cutting the samples,  the serrations and undercuts should   be  ground  and the specimen should be ground to a 120-grit finish. Under all circumstances use new blades and avoid mix up with blades cutting C.S or LAS.

 

 

The  test for welded coupons  is  required to be done in as welded conditions, thus the above guidelines would be of help. I have a attached an article on  G-48 test and it’s implications.

 

Thanks.

 

 

Pradip Goswami,P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

-----Original Message-----

From: materials-welding@googlegroups.com

[mailto:materials-welding@googlegroups.com] On Behalf Of Sudhakar

Sent: Monday, June 28, 2010 8:43 PM

To: materials-welding@googlegroups.com

Subject: [MW:5772] ASTM G 48 testing for SDSS

 

Dear members,

 

What are the extra special precautions that need to be taken for conducting ASTM G48 Method A test @ 40 deg C for A 790 UNS 32750 material.

 

Rgds

Sudhakar

 

Sent from my iPhone

 

--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to

materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at

http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and

meant for educational purposes only, Users must take their own decisions

w.r.t. applicable code/standard/contract documents.

 

 

 


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

 

 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...