RE: [MW:5236] Repaire of Damaged Galvanised Sheet

1. What caused the White Rust? If the causes are not eliminated it will
re-occur
2. How much White rust?
3. How mush of teh orginal galvanizing remains? (Measure the thickness with
a device like a Positech 6000)
4. If sufficnet Galvanizing remains the white rust can be removed by a
stiff brush (Plastic or brass Not Steel).
5. Individual sheets are cut from rolls of galavized material,
re-galvanizing a complete sheet muight be possible in a Hot-Dip tank.
6. there are several methods for repairing, eithar a cold zinc rich paint
system applied to the surface of a Tin/Zinc solder based solder applied
with heat.

To make a paint repair look acceptable , paint the surface, when partially
dry use a scotchbrite (
http://img.epinions.com/images/opti/dc/d0/Scotch-Brite_Heavy_Duty_Scour_Pads
-resized200.jpg
) cleaning pad to blend the surrounding area.

Life - depends on envirnomental conditions.

Best Regards,

Richard M. Beldyk PhD, PE, MIET
AWS Certified welding Engineer
ASQ Certified Six Sigma Black Belt


Original Message:
-----------------
From: Mrityunjay Kumar / ZS Saudi PEB QA/QC Mrityunjaykumar@zamilsteel.com
Date: Mon, 24 May 2010 14:49:13 +0300
To: materials-welding@googlegroups.com
Subject: [MW:5230] Repaire of Damaged Galvanised Sheet

Dear Friends,
Please advise me whether

1. we can repair the white rusted GI sheet (Thick 1 - 3.00 mm, ASTM
A653, Gr-S340)

2. or can we re-galvanize the sheet

3. or for few spots, shall we use some spray but for this A) How to
clean B) its life & C) visual appearances

Best Regards,
M.K.Choudhary
[cid:image001.png@01CAFB4F.6CB12FA0]
P.O. Box 877, Dammam 31421 KSA
Phone : (+9663) 8471840 X 555
Fax : (+9663) 8471291
www.zamilsteel.com

----------------------------------------------------------------------------
----------------------------
Disclaimer: This email and any files transmitted with it are confidential
and intended solely for the use of the addressee(s) named herein. If you
are not the intended recipient or addressee, you should not use,
disseminate,
distribute, copy or alter this email. Any views or opinions presented in
this
email are solely those of the author and might not represent those of
"Zamil
Industrial" and or its units.

Warning: Although reasonable precautions have been taken to ensure no
viruses
are present in this email, the company cannot accept responsibility for any
loss or damage arising from the use of this email or attachments. If you
have
received this electronic mail message in error, please contact the sender
directly.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.


--------------------------------------------------------------------
mail2web LIVE – Free email based on Microsoft® Exchange technology -
http://link.mail2web.com/LIVE


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...