Applying conventional PWHT on this case is a very dangerous thing to do.
This is a design issue. The designers must know these issues.

2205 (2209) Duplex stainless steel (overlay) will not tolerate any prolonged exposure above 600F without forming detrimental secondary phases. It is not a risk, it is guaranteed to destroy the corrosion resistance (and impact toughness) of DSS. Yet, you can prepare a test coupon and simulate everything and send it for laboratory tests to see for yourself. 

You have to forget about PWHT or go for a sold DSS vessel.
There are not many other alternatives which can completely fix this issue for you.   

Regards
Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Sun, Jul 19, 2020 at 1:42 PM Umar Rashid Makrani <firoz.makrani@gmail.com> wrote:
Respected Sir,
We value your various inputs on our queries and many of us are much thankful for this. No doubt your professionalism is useful for the welding community. Your supports to all of us on various cases was unprecedented. 
There may be time when we might not been convinced to your answer, we should rather repeat the queries or present the counter arguments in a better respectful way with a proper technical/scientific clarifications. The respect is due to all the community heroes like you.
Yes we agree that pressure vessels are not the cookies and deserve respect too, we don't want to repeat the Bhopal nor even a single unrecorded injury.
Thank you very much to all the experienced mentors of the group and we expect that we will be forgiven for any unprofessional comment we may make out of our ignorance.
Best regards,

On Sunday, July 19, 2020 at 6:33:45 AM UTC+3, pgos...@rogers.com wrote:

Hello Sourav,

 

I'm not sure what you're trying to convey. However what you're writing does not make any sense at all.

Pressure vessels are not cookie cutters, they're serious and dangerous equipment.  You can't just weld, put inside the furnace and attach a few thermocouples…….. and be done…

I'm attached to this forum for last 10 years and have initiated and contributed many in-depth  technical issues.

If you're interested to know something, let me know. I'll gladly  help you.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:p...@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: Sourav Bohrays <sourav...@gmail.com>
Sent: July 18, 2020 7:53 AM
To: material...@googlegroups.com
Subject: Re: [MW:31152] CS with Duplex SS (S31803) clad vessel PWHT?

 

i am not getting why you are sooo afraid of cladding with cs .you have to do nothing especial for this simply put your job in  close furnance and attached weld but remember if u are attaching thermocouple inside of vessel also than dont weld it at ss plate ,attach it at weld.i i did firing in furnace not inside the remember if its not clad than i have a option of inside firing of vessel

 

On Sat, 18 Jul 2020, 8:01 am , <pgos...@rogers.com> wrote:

A few questions on this interesting  topic  as well as  on the suggestions imparted as below.

 

  • How  do you perform local PWHT on a fully fabricated pressure vessel? If that's the case , every weld joint (L-Seam, C-Seam, Nozzle Welds ) has to be individually wrapped by heating coils. Is that possible  after fabrication of entire vessel?
  • Restoration of Duplex clad is usually done after barrier layer by 309L.  2209 electrode/filler  may be used  also right from the first layer for restoration of clad.  
  • PWHT of 51 mm thick Duplex clad vessel would encompass the following PWHT cycle easily:-
  1. Ambient to 300 Deg C-Unlimited heating, 300 Deg C /Hr. Hold at 300 Deg c for uniform equalization of  temperature
  2. From 300 Deg C to 600 Deg C – ROH 40-50 Deg C /Hr- would involve- easily 4 hrs of heating cycle
  3. Soak 2 600-620 Deg C- for 2 hrs easily

Hence depending on the size of the vessel, a heating cycle of 7-8 hrs easily would be required between 300- Deg C  to 600 Deg C. Same would be case for cooling . Hence a PWHT .stress relief temperature @ 600 Deg C  could be quite harmful. Typically 300-700 Deg C is the formation range of various intermetallic phases for Duplex S.S.

 

It would be nice to know the decision taken by the originator of this query , for education of all concerned.

 

Thanks.

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:p...@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: material...@googlegroups.com <material...@googlegroups.com> On Behalf Of Customer Care
Sent: July 11, 2020 10:13 PM
To: material...@googlegroups.com
Subject: RE: [MW:31136] CS with Duplex SS (S31803) clad vessel PWHT?

 

Hi,

You can realize the dissimilar welding (CS 516 Gr.70) + Cladding (S31803) with PWHT following these steps:

-As the base metal of CS have 51 mm of thickness, apply preheating about 175 °C and maintain it during the welding.   Use filler for CS type E/7018 (depending welding process).

 

-Buttering the CS with austenitic filler metal (e.g., E/309L) and remove clad S31803 with grinding, 2" side and side of the weld joint. Realize localized PWHT over the weld metal and HAZ only, about 625 °C during one and half hours.

             - Weld the S31803 clad using duplex filler like E/2209.

 

Ramon Briceno

Senior Metallurgical Engineer / Oil & Gas

 

 

Sent from Mail for Windows 10

 

From: Materials & Welding
Sent: Saturday, July 11, 2020 6:42 AM
To: Materials & Welding
Subject: [MW:31131] CS with Duplex SS (S31803) clad vessel PWHT?

 

ASME Sec VIII div1

SA516 Gr 70 - 51mm thickness+S31803 clad

 

any experience on duplex clad vessel PWHT?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d1dd74b8-9481-47ce-a896-8d41a29c527cn%40googlegroups.com.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BL0PR03MB42430F71AF631FA12E6C9631AA630%40BL0PR03MB4243.namprd03.prod.outlook.com.

 

Virus-free. www.avg.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAACMA%2BVkArTCRJUPEAxMCRVJAQAAAAA%3D%40rogers.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1f9668e1-33ea-4496-b481-19ad4c03dd5co%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEagfUhLZ6FRw5arrA5zkX%3DMjry7xehSjNM%3Drkea4Sid5zxbkA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...