A few questions on this interesting  topic  as well as  on the suggestions imparted as below.

 

  • How  do you perform local PWHT on a fully fabricated pressure vessel? If that's the case , every weld joint (L-Seam, C-Seam, Nozzle Welds ) has to be individually wrapped by heating coils. Is that possible  after fabrication of entire vessel?
  • Restoration of Duplex clad is usually done after barrier layer by 309L.  2209 electrode/filler  may be used  also right from the first layer for restoration of clad.  
  • PWHT of 51 mm thick Duplex clad vessel would encompass the following PWHT cycle easily:-
  1. Ambient to 300 Deg C-Unlimited heating, 300 Deg C /Hr. Hold at 300 Deg c for uniform equalization of  temperature
  2. From 300 Deg C to 600 Deg C – ROH 40-50 Deg C /Hr- would involve- easily 4 hrs of heating cycle
  3. Soak 2 600-620 Deg C- for 2 hrs easily

Hence depending on the size of the vessel, a heating cycle of 7-8 hrs easily would be required between 300- Deg C  to 600 Deg C. Same would be case for cooling . Hence a PWHT .stress relief temperature @ 600 Deg C  could be quite harmful. Typically 300-700 Deg C is the formation range of various intermetallic phases for Duplex S.S.

 

It would be nice to know the decision taken by the originator of this query , for education of all concerned.

 

Thanks.

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Customer Care
Sent: July 11, 2020 10:13 PM
To: materials-welding@googlegroups.com
Subject: RE: [MW:31136] CS with Duplex SS (S31803) clad vessel PWHT?

 

Hi,

You can realize the dissimilar welding (CS 516 Gr.70) + Cladding (S31803) with PWHT following these steps:

-As the base metal of CS have 51 mm of thickness, apply preheating about 175 °C and maintain it during the welding.   Use filler for CS type E/7018 (depending welding process).

 

-Buttering the CS with austenitic filler metal (e.g., E/309L) and remove clad S31803 with grinding, 2" side and side of the weld joint. Realize localized PWHT over the weld metal and HAZ only, about 625 °C during one and half hours.

             - Weld the S31803 clad using duplex filler like E/2209.

 

Ramon Briceno

Senior Metallurgical Engineer / Oil & Gas

 

 

Sent from Mail for Windows 10

 

From: Materials & Welding
Sent: Saturday, July 11, 2020 6:42 AM
To: Materials & Welding
Subject: [MW:31131] CS with Duplex SS (S31803) clad vessel PWHT?

 

ASME Sec VIII div1

SA516 Gr 70 - 51mm thickness+S31803 clad

 

any experience on duplex clad vessel PWHT?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d1dd74b8-9481-47ce-a896-8d41a29c527cn%40googlegroups.com.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BL0PR03MB42430F71AF631FA12E6C9631AA630%40BL0PR03MB4243.namprd03.prod.outlook.com.


Virus-free. www.avg.com

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...