Re: [MW:30783] hello

Alloy 800 HT could not be the right material above 1560 deg F.
Normally metal dusting occurs in range of 1100-1350 deg F.
Choice of Alloy 699 , 601 or 602 CA could be right choice in this temperature range.

Could you please tell who is the process licencor pf reformer ?

Best Regards
Atul Khatri

On Thu, Apr 16, 2020 at 8:56 AM Hernan Arturo Castillo Mier <Hernan.Castillo@ecopetrol.com.co> wrote:

 

Thanks,

 

Temperature is about 1600°F

Thermowells are installed in a boiler downstream the reformer.

On the other hand, see the corrosion present in the bypass duct before the damper downstream the boiler.

 

Yes, its metal dusting.

Look at the pictures attached  (confidential)

 

 

De: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] En nombre de atul khatri
Enviado el: miércoles, 15 de abril de 2020 12:12 AM
Para: materials-welding@googlegroups.com
Asunto: Re: [MW:30758] hello

 

Hi Hernan,

Could you please give some more details ?

What is the temperature of your reformed gas ?

Are you sure it's because of metal dusting ?

What does your licencor says ?

 

 

Hope I can help you after your replies . 

 

Br,

Atul 

 

 

On Wed, Apr 15, 2020 at 9:19 AM Hernan Arturo Castillo Mier <Hernan.Castillo@ecopetrol.com.co> wrote:

We have metal dusting corrosion in two thermowells, downstream of Hydrogen reformer.

Any have experience about this problem?

Thermowells are Incolloy 800HT.  This is not the best metallurgy for this corrosion problem.

According to NACE, the better metallurgy is Alloy 699 XA.

We are looking for any factory that  produce thermowells using that metallurgy.

 

Thanks,

 

 

Hernán Castillo Mier

Senior Engineer

Reliability and integrity of Static equipments.

API 510 (33119)

Ecopetrol   Cartagena Refinery

Este mensaje puede contener información de tipo personal, clasificada o reservada; si usted no es el destinario, por favor, hacer caso omiso de su contenido y abstenerse de compartirlo, reenviarlo o copiarlo. Si recibe este mensaje por error, agradecemos informarlo inmediatamente al remitente y borrarlo permanentemente de su cuenta. Si usted está autorizado para recibir la información de tipo personal, se le recuerda que esta información debe ser manejada con la finalidad con la que ha sido solicitada y en virtud de la normativa que habilita el acceso a la misma. Así mismo, deberá ser usada bajo los parámetros de la ley 1581 de 2012 de protección de datos personales y la normativa que la desarrolla, siendo responsabilidad del área receptora del cumplimiento de la citada normativa de protección de datos personales. CONFIDENTIALITY NOTICE: This electronic transmission (including any files attached hereto) (this "Communication") contains information that is or may be legally privileged, confidential, and exempt from disclosure without our express permission in advance. The information is intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient or any employee or agent responsible for delivering the message to the intended recipient, you are hereby notified that any disclosure, dissemination, copying, distribution, or the taking of any action in reliance on the contents of this electronic Communication is strictly prohibited. If you have received this Communication in error, please notify the sender immediately and destroy permanently the transmitted information in its entirety and do not disclose its contents to any other person. Para conocer la Declaración de Tratamiento de Datos Personales de Ecopetrol, favor consultarla en www.ecopetrol.com.co Responsabilidad Corporativa – Declaración de Tratamiento de Datos Personales.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BN6PR22MB089956FA0C517B388C82708DDDDA0%40BN6PR22MB0899.namprd22.prod.outlook.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACKOSeDXJNaA3cF2kwGmZTUtGw5cTqZtKOveC7Q2YW%3DgwVVVpg%40mail.gmail.com.

Este mensaje puede contener información de tipo personal, clasificada o reservada; si usted no es el destinario, por favor, hacer caso omiso de su contenido y abstenerse de compartirlo, reenviarlo o copiarlo. Si recibe este mensaje por error, agradecemos informarlo inmediatamente al remitente y borrarlo permanentemente de su cuenta. Si usted está autorizado para recibir la información de tipo personal, se le recuerda que esta información debe ser manejada con la finalidad con la que ha sido solicitada y en virtud de la normativa que habilita el acceso a la misma. Así mismo, deberá ser usada bajo los parámetros de la ley 1581 de 2012 de protección de datos personales y la normativa que la desarrolla, siendo responsabilidad del área receptora del cumplimiento de la citada normativa de protección de datos personales. CONFIDENTIALITY NOTICE: This electronic transmission (including any files attached hereto) (this "Communication") contains information that is or may be legally privileged, confidential, and exempt from disclosure without our express permission in advance. The information is intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient or any employee or agent responsible for delivering the message to the intended recipient, you are hereby notified that any disclosure, dissemination, copying, distribution, or the taking of any action in reliance on the contents of this electronic Communication is strictly prohibited. If you have received this Communication in error, please notify the sender immediately and destroy permanently the transmitted information in its entirety and do not disclose its contents to any other person. Para conocer la Declaración de Tratamiento de Datos Personales de Ecopetrol, favor consultarla en www.ecopetrol.com.co Responsabilidad Corporativa – Declaración de Tratamiento de Datos Personales.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BN6PR22MB089992F9D7E311A192F13B90DDDB0%40BN6PR22MB0899.namprd22.prod.outlook.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACKOSeCthqXm1jm0x%3DM8qP%2BRF1vA%3DKTdqQmQWvpbw77vX%2BfoDQ%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...