Higher hardness could mean:
Higher residual stresses
Martensite formation
The most probable cause are Higher residual stresses. 
To reduce the residual stresses are following options:
1. Increase preheat. You may try 100degC
2. Decrease interpass temperature. You May try 150 degC
3. Decrease heat Input by shortening the arc or Increase welding spead

Στις Πέμ, 9 Απρ 2020, 13:31 ο χρήστης 'dwh@btinternet.com' via Materials & Welding <materials-welding@googlegroups.com> έγραψε:


Try a slower welding speed and a closer arc length.

Regards, 9 4 2020.

David Harvey

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/3277447a.10ad.1715e7c63d8.Webtop.227%40btinternet.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40AHVffPV6MKS_tuw0gDMjYupCC7Cj0U_-i0G8QK0F0nUg%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...