Re: [MW:29369] WELDING DEFECT AT ROOT

Its a LOP . If you have access to repair from inside, otherwise cut the root.
RT is not showing, I think that area have litter excess reinforcement than other.

On 24 Mar 2019 7:48 am, "George Dilintas" <dilintas@gmail.com> wrote:
If the edges of the root gap are nor fused, then it is not simply root concavity, it is lack of penetration. Are you sure that the root egdes of the Base metal are fused

Στις Παρ, 22 Μαρ 2019, 00:28 ο χρήστης Muhammed Ibrahim PK <ibratech@gmail.com> έγραψε:
Gents, 

I am getting the attached image in boroscope inspection at root. But RT not showing any density variation or undercut. Please give your comment on it. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...