[MW:29407] Re: PMI Testing -ss316

Hello,

Plate ASTM A240 TP316: refer tolerance in ASTM A480 Table A1.1
Pipe ASTM A182 TP316, refer tolerance in ASTM A961 Table  1.

>Tolerance: Ni 0.15% content 

So, Ni reading 9.86% is acceptable.

Regards
Bien ND

On Thursday, March 28, 2019 at 5:14:08 PM UTC+7, Sameer wrote:
Dear Experts ,
During PMI testing of SS316 material Ni observed - 9.86% , required range is 10-14%.
observed value will be accepted or not . Please provide your valuable comments .

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...