Re: [MW:24984] IMPACT TEST REQUIREMENT

No, if you read carefully the last sentence of 5th paragaphe of QW-403.5 the combination in the same test coupon qualifies the group numbers to themselves.
However if the application Code Section (VIII-1, VIII-2) does not require HAZ impact testing you dont have to worry about this variable

2016-06-18 12:11 GMT+03:00 'Mohammed Rafiuddin' via Materials & Welding <materials-welding@googlegroups.com>:
PQR on P1Gr1 to P1Gr2 qualifies welding P1Gr1 to P1Gr2 only and NOT welding to themselves i.e ( P1Gr.1 To P1Gr1 Or P1Gr2 to P1Gr2)

Refer ASME interpretation IX-92-70 on the same subject.I could not find downlodable copy.Try to search on internet.

Thanks
Mohammed


On Friday, 17 June 2016 1:52 PM, "nithindsilva4u@gmail.com" <nithindsilva4u@gmail.com> wrote:


P1 G1 to P1 G2 qualifies P1 G1 to P1 G2, P1 G2 to P1 G2 and P1 G1 to P1 G1. Hope your query is addressed.

Sent from my iPhone

On Jun 17, 2016, at 11:37, balaji srinivasan <bolukbalaji@gmail.com> wrote:

Dear All,


As per ASME SEC-IX   change in material Group is Supplementry  essential variable (403.5)

based on above i need your experience  If iam qualified PQR p1 group-1 to p1 group-2 tow different group welded it self so the  qualfied range will be p1 group1 and p1 group 2.

or only this PQR is qualified group 1 to group-2 qualified.

also please advice i need to qualify group 1 separate and group 2 separate PQR.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAK1csg3Drkobg2%3DG9Lyy0CMd3WbM%2BOq_9e2GkJLoC-QxBUhP0A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0232776F-14AF-4FF0-8B7E-DA998585BF07%40gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/492345405.4017979.1466241063907.JavaMail.yahoo%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CAYkD_Ub6S4gpgeFS-a4yyb_rZ4VaDSAvsMkev514APQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...