Dear Sir,
There is no change in P No.
Please give me the reason with reference to ASME BPVC Sec IX.

Regards,

Hareesh K V

On Jun 16, 2016 10:25 AM, "Lalu Rajendran" <lalucpt@gmail.com> wrote:
​Yield value of 410S is 30 ksi​. 

On Wed, Jun 15, 2016 at 7:40 PM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:

What about strength?

On 15-Jun-2016 4:31 pm, "Lalu Rajendran" <lalucpt@gmail.com> wrote:
Austenitic consumables (E309L) can be used for SS 410S material for temperature below 600 deg C due to sigma formation (Brittle phase) in the welds. Also PWHT can be avoided if you use E309L.

regards,
LALU 

On Wed, Jun 15, 2016 at 10:43 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
change in Pno is essential variable.

For P7toP7, why 309L?

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Jun 15, 2016 at 8:33 AM, makrand sakpal <makrands9@gmail.com> wrote:

Is there any specific reason?

On 14-Jun-2016 12:13 pm, "Lalu Rajendran" <lalucpt@gmail.com> wrote:
Hi,

No, You must qualify a separate PQR for P7 to P7 with ER 309LMo.

regards,
LALU

On Tue, Jun 14, 2016 at 5:33 AM, Hareesh K V <hareesh13h@gmail.com> wrote:
Dear all,

we have qualified a PQR (groove weld) for clad material (SA 240 410S (Clad) to Carbon Steel that is P7 to P1 material) using ER 309L Mo for the clad portion and E7018 for the rest.

Now we have to weld SA240 410S to SA240 410 S material for another job.

My question is, can we use the above said qualified PQR to make a wps of SA240 410S to SA240 410 S material, as other variables are same.

Thanking you,

Hareesh K V
+91-9447625012


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM3LgAVu5WdYUooGcah4gsV5LR3F8z9Se8JLoNnJgaGZE9hmFw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13vfLBhfkG5wdiuM2oVXbpiHz3v3ETk_qY3tFfFkZ2o4_A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKJec9L0hMRM7HDoXL2B6OksgYf8Qq%3DXTKNgc4gm67VTg2Sc_w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNsOWo8W%2BHVV9oZ8MUbAjdOKBAM3C66mpwaqRaN0v738Q%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13seFrwpch6E_sZD8bBWCYG4%3Dh8ZmU2Mn%3DQ4avP7zrZYdg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eMaA6wKsJXauYO0QRnBqg4%2BfUSLRantqt2SrvcwtmEvjw%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13sxd4vJChkj_3L1WfzEaBSnAzsb188d1YCKcutNynGRYw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM3LgAVNiDoo_4fYnBy0ziQ79XUZWbZZv%2BvGNFeucVE0erQdeQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...