Monday, May 23, 2016

RE: [MW:24837] Hardness issue on weld metal

Asume Conde B31.3 in PWHT section  is ndicated  what time and temperature fdoyou need for making stress relief.

Specif section un this moment I can not tp tell you.

Also you hace todo consider Asme Conde VIII snd Asume Conde IX

El 23/05/2016 08:57, "Jim Price" <JimPrice@polarcorp.com> escribió:
Boxbe This message is eligible for Automatic Cleanup! (JimPrice@polarcorp.com) Add cleanup rule | More info

At what temperature was PWHT, holding time, cooling rate.

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimprice@polarcorp.com

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sathish Kumar
Sent: Friday, May 20, 2016 3:56 AM
To: Materials & Welding
Subject: [MW:24816] Hardness issue on weld metal

 

Dear Experts
We have recently welded 1/2" thick and 1" Thick pipes, Material : AISI 4130. Our hardness requirement is 197BHN-237BHN

This pipes are groove welded to same size of the pipes, Followed by GTAW(ER100S-G) & SMAW(E10018-D2) process. Root is followed by GTAW and SMAW for fill up and capping.on completion of PWHT we observed following hardness value.




After completion of welding and PWHT, we have found hardness range of 285HBN and 265HBN on weld metal. Also we performed PMI on the weld metal to determine the hardness issue, during the result we found following chemical composition on the weld metal respectively.

 

Tabulation shows actual chemistry of the T.C

 

Chemistry observed as per the T.C

 

Size

C

Mn

Si

S

P

Cr

Ni

Mo

V

Cu

 

E10018-D2

3.2mm

0.074

1.980

0.550

0.009

0.022

 

0.460

0.400

 

 

 

4mm

0.068

1.940

0.510

0.008

0.021

 

0.690

0.370

 

 

 

5mm

0.062

1.980

0.470

0.009

0.019

 

0.630

0.340

 

 

 

 

 

Tabulation shows actual chemistry after PMI inspection

 

CHOKE & KILL Line

 

Chemistry observed as per the PMI

Other metals

Weldment area

C

Mn

Si

S

P

Fe

Cr

Ni

Mo

V

Cu

Ti

 

On Weld Metal 90°

 

2.00

 

 

 

95.33

0.047

0.807

0.486

0.03

0.024

1.2667

 

On Weld Metal 180°

 

1.966

 

 

 

96.616

0.033

0.838

0.486

0.00

0.058

0.00

 

On Weld Metal 270°

 

2.060

 

 

 

96.443

0.057

0.902

0.492

0.00

0.044

0.00

 

On Weld Metal 360°

 

2.115

 

 

 

96.401

0.363

0.907

0.501

0.00

0.037

0.00

 

 

 

 

BOOSTER Line

 

Chemistry observed as per the PMI

Other metals

Weldment area

C

Mn

Si

S

P

Fe

Cr

Ni

Mo

V

Cu

Ti

 

On Weld Metal 90°

 

1.946

 

 

 

95.287

0.150

0.915

0.500

0.021

0.150

1.113

 

On Weld Metal 180°

 

1.992

 

 

 

96.362

0.152

0.932

0.491

0.00

0.152

0.00

 

On Weld Metal 270°

 

0.203

 

 

 

96.303

0.203

1.121

0.490

0.00

0.203

0.00

 

On Weld Metal 360°

 

0.252

 

 

 

96.556

0.252

0.735

0.480

0.00

0.252

0.00

 

 

On comparison of chemistry for actual observed in the T.C and PMI result varies accordingly, those variation exceeds the standard requirement of ASME Sec II part-C. Those variation are tabulated for your reference, also PMI is taken on the undiluted weld metal of the capping.

 

We suspect that due to exceed of Mn and Ti, hardness increased. Please suggest or advice on the following issues.

 

 

NOTE-

Interpass Temperature maintained: 300°C

Preheat Temperature maintained: 210°C



Regards
S.Sathish kumar

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7fa8ee58-6ea4-4734-a6dc-1866048fe626%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f5d3dbe5ec204e5d95a49eb9f4600309%40POLARMAIL.PolarTank.local.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACeZn86rJRrLsqeQbexpNb5iYn3Q0gnDUNv3vcGobwUcJinHkg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...