Re: [MW:24015] IMPACT EXEMPTION FOR DUPLEX FLANGES SA 182 Gr F51

Dear vish


In UCS-66 the governing thickness is important factor cause we have combination of minimum design metal temperature
 and governing thickness to the subject material. 

but in UHA-51 impact test requirement is based on the material properties and material thickness is not an essential variable . (except where noted)

UHA-51 IMPACT TESTS
Impact tests, as prescribed in (a),shall be performed
on materials listed in Table UHA-23 for all combinations
of materials and minimum design metal temperatures
(MDMTs) except as exempted in (d), (e), (f), (g), (h),or
(i). 


Best regards.

-------------------------------

On Monday, December 28, 2015 at 10:59:30 AM UTC+3:30, Vish wrote:
Thanks MW,

But my question remains same that, what will be nominal thickness of duplex flanges to be consider ?
 

vish

On Thursday, December 24, 2015 at 2:58:57 PM UTC+5:30, MW wrote:
i guess you should use Appendix JJ, 
UHA -51(g)?


On 24 December 2015 at 13:11, VISHNU <vishnu...@gmail.com> wrote:
Dear sir,

I have one query regarding to above subject,

One of the definition of governing thk when using fig. UCS-66 - Governing thickness of flat non welded parts, such as bolted flanges, tubesheet and flat head is the flat component thickness divided by 4

But what about Duplex flanges ? UHA is not giving such clause, so what will be governing thickness to be consider for duplex flanges (SA 182 F51) ?

Thanks in advance

Regards

vishnu 


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e38957c7-58ab-4ad1-a378-e7a7732f8c36%40googlegroups.com.