Material specification: SA333 Gr.6
Impat requirement: Yes at -45 °C
PWHT: No.
Job thicknesses: 6.35mm, 7.92mm,8.56mm, 9.52mm,10.97mm,11.33mm,14.27mm, 15.88mm, 19.05mm,25.4mm
PQR 1) GMAW- 6.35mm
Root pass by short circuit mode- 3mm
Subsequent passes up to capping by pulsed spray mode-3.35mm
PQR 2) GMAW- 14.27mm
Root pass by short circuit mode- 3mm
Subsequent passes up to capping by pulsed spray mode- 11.27mm
WPS for above thicknesses,
Reference PQRs: PQR 1) & PQR 2)
In WPS- Base metal T range: 6.35mm to 12.7mm & 14.27mm to 28.54mm.
Weld metal t GMAW-Short circuit: 3.3mm
Weld metal t GMAW-Pulsed spray: 22.54mm
Reference Document: ASME sec.IX
a) QW403.10 GMAW short circuit mode T is 1.1T
b) QW404.32 GMAW short circuit mode t is 1.1t.
c) QW 403.6 for impact requirement.
Question 1)
above WPS T & t value is correct??, if not correct me with justification.
Question 2)
GMAW process remains same for making WPS with short circuit & pulsed spray mode
Note:We don't have thickness range between 11.33 to 14.27mm
Regards,
Pravin Nimbalkar
Welding Engineer
+966577620240
What's app: +919975724942
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e00ac9b8-c314-4428-bd06-ef155ba0411d%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment