Sunday, December 15, 2013

Re: [MW:19603] Effect of grinding on ferrite content in urea service

BEGIN:VCARD
X-LOTUS-CHARSET:UTF-8
VERSION:3.0
PRODID:-//Lotus Development Corporation//NONSGML Notes 8.5.2//EN_C
FN:George H Dilintas/GRC/VERITAS
N:Dilintas;George;;;
ADR;TYPE=WORK;TYPE=PREF:PIRAEUS;;23\, Etolikoy Str.;PIRAEUS;;185 45
;GREECE
ADR;TYPE=HOME;TYPE=PREF:;;19-21 B. Laskou str.;Athens;Attika;11 633
;Greece
TEL;TYPE=HOME:+30-1-7667 197
TEL;TYPE=WORK:+30-210-40 63 113
TEL;TYPE=HOME;TYPE=FAX:+30 - 1 - 7667 197
TEL;TYPE=WORK;TYPE=FAX:+30-210-40 63 118
TEL;TYPE=CELL:+30 -69 44-64 62 04
EMAIL;TYPE=WORK;TYPE=PREF;TYPE=INTERNET
:george.dilintas@gr.bureauveritas.com
ORG:Bureau Veritas;Industry
REV:20131201T024559Z
END:VCARD

Do you mean Iron contamination?

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

Hrushikesh Sangamnerkar ---15/12/2013 09:47:43---Dear all I would like to know what is effect on ferrite due to grinding. I have

From: Hrushikesh Sangamnerkar <hrushi612@gmail.com>
To: materials-welding@googlegroups.com
Date: 15/12/2013 09:47
Subject: [MW:19598] Effect of grinding on ferrite content in urea service
Sent by: materials-welding@googlegroups.com




Dear all

I would like to know what is effect on ferrite due to grinding. I have heard and also practically observed it that grinding tends to increase the ferrite content. Also its not permitted on job. But I dont have any references. Kindly share your experience if any.

Base metal- SA 240 type 310
Filler metal - 25.22.2 LMn
Process - GTAW
Thickness - 5mm

Thanks and regards
Hrushikesh H Sangamnerkar

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...