Dear,

Standard: SSPC PA 2

5.2.1 Minimum Thickness: The average of the spot measurements for each 10 m2 (100 ft2) area shall not be less
than the specified minimum thickness. No single spot measurement in any 10 m2 (100 ft2) area shall be less than 80% of the
specified minimum thickness. Any gage reading may under-run by a greater amount. If the average of the spot measurements
for a given 10 m2 (100 ft2) area meets or exceeds the specified minimum thickness, but one or more spot measurements is less
than 80% of the specified minimum thickness, additional measurements may be made to define the non-conforming area.

5.2.2 Maximum Thickness: The average of the spot measurements for each 10 m2 (100 ft2) area shall not be more
than the specified maximum thickness. No single spot measurement in any 10 m2 (100 ft2) area shall be more than 120% of the
specified maximum thickness. Any gage reading may over-run by a greater amount. If the average of the spot measurements
for a given 10 m2 (100 ft2) area meets or falls below the specified maximum thickness , but one or more spot measurements is
more than 120% of the specified maximum thickness, additional measurements may be made to define the non-conforming
area. Manufacturers’ literature may be consulted to determine if higher maximum thickness readings are allowable under
specific circumstances.

Also you can see ASTM D 1186

There may be no. of reasons for failure in test.

What was required DFT ?

What was the max DFT observed ?

What is the average DFT observed ?

For Proper Pull Off test refer ASTM D3359

Test Method A—An X-cut is made in the film to the substrate, pressure-sensitive tape is applied over the cut and
then removed, and adhesion is assessed qualitatively on the 0 to 5 scale.

Test Method B—A lattice pattern with either six or eleven cuts in each direction is made in the film to the
substrate, pressure-sensitive tape is applied over the lattice and then removed, and adhesion is evaluated by comparison with descriptions and illustrations.


Test Method A is primarily intended for use at job sites while Test Method B is more suitable for use in the laboratory.
Also, Test Method B is not considered suitable for films thicker than 5 mils (125μm).



On Wed, Sep 26, 2012 at 12:47 PM, Ramchandra vichare <vicharerke@indiatimes.com> wrote:
Dear Experts;

with reference to the subject referred above please let me advise with documentary evidence about tolerances for  Painted items when DFT is specified. Why paining fail in cross cut/peel-off test(Pl. ref photograph attached)? How to control the same?

Requested to advise

Regards
RK Vichare

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...