Re: [MW:15404] Welding consumable for welding of CS to Cast Iron


Mr. Ranendra Chakraborty,
 
E Ni-Fe-CI with 45% Ni generally recommended for repair welding of CI. 
E Ni-CI with 98% Ni is also recommended for repair welding of CI.
E Ni-Cu B with 70% Ni(+) Cu could be used for repair welding of CI. 

Welds done with above electrodes are machinable and are Ok for CI (+) MS welding except that, due to NI addition,we can not expect colour matching.

The cost factor of the electrodes are high.

E St-Low Hydrogen type electrode could be used for repair welding of CI and CI to MS. 
Colour matching is good, but non machinable and preheating to en extent of 350 deg and above are required.

On same basis, you can use E7018, E7016, E8018-G (with1.25% Ni addition) for welding CI to MS. All are moderately priced.

In all  the cases, peening (short hammering) of each weld bead layer is recommended to avoid stress concentration which will lead to cracking during welding.

Sridhar.
--------------------------------------------------------------------------------



From: Srinivasan Jagannathan <jsrisud@gmail.com>
To: materials-welding@googlegroups.com
Sent: Tuesday, 25 September 2012 8:44 PM
Subject: Re: [MW:15394] Welding consumable for welding of CS to Cast Iron

Dear All,  That's the correct recommendation,  I have seen many times in this forum people misusing the forum to abuse other's products and promote their products especially some so called "REPUTED " companies.

Hats off to Mr.Saleem for giving a codified product as solution than giving a brand & promoting it.

J.Srinivasan



On Tue, Sep 25, 2012 at 7:05 PM, hesham seleem <heshamseleem7@hotmail.com> wrote:
Dear Sir

Regarding To Your Question about welding CS to DI-Electrode Used is

AWS A5.15: ENIFe-c1

DIN 8573: ENIFe-1  BG13



Date: Tue, 25 Sep 2012 17:36:01 +0530
Subject: [MW:15391] Welding consumable for welding of CS to Cast Iron
From: ranendrac6@gmail.com
To: materials-welding@googlegroups.com


Dear Experts,
Please guide which kind of consumable can be used for welding of CS with Cast Iron.
 
Ranendra Chakraborty

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 



--
J.SRINIVASAN

GENERAL MANAGER - TRAINING

D&H SECHERON - INDORE

Mob: 7898989756

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...