Hi
 
Its not an easy task to weld Al bronze.
What is your base material grade ?
Clean base metal and filler wire before welding. 
Use 99.995% pure argon.
Preheat 150 – 180 ˚C
Inter pass temperature @200 ˚C.
Inter run cleaning is very important to remove surface oxides 
 
Regards
 
Prem Nautiyal
Cell: 9769316004
 
--- On Fri, 9/21/12, bo gyi <aungbomyint@gmail.com> wrote:

From: bo gyi <aungbomyint@gmail.com>
Subject: [MW:15353] Aluminium Bronze welding
To: materials-welding@googlegroups.com
Date: Friday, September 21, 2012, 7:46 AM

Hi Sirs,

Currently, I am doing procedure for Aluminium Bronze (61400) using GTAW ( ERCuAl-A2) process by Argon shielding gas but found that fusion of filler metal & base metal is not nice.

Can anyone advice?

Thanks and regards,

Bo 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...