Friday, July 1, 2011

Re: [MW:11561] SA82 F316L Flanges

Dear Kumar,
 
Heat Treatment is required as it is mentioned in SA 182 (Table - 1) of SEC II Part A - Begining.
 
For 316L 1040°C is the required Temp followed by water quenching.
 
 
Regards,
Shivkumar
Alfa Laval India Ltd.
On Wed, Jun 29, 2011 at 7:57 PM, narayanasamy kumar <avenkumar@yahoo.com.sg> wrote:
Dear Experts,
           
            Can anybody tell SA 182 F316L 1" Flanges we received without Solution annealing, Is it acceptable? Please let me know code reference.(ASME SEC II A).
 
Thanks and Regards,
Kumar.
Singapore.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35346] Cast-iron welding

Any advice for cast iron welding Sent from Yahoo Mail for iPhone