[MW:1975] RE: 1964] FW: 1963] SS 410 overlay with E 309L MO barrier layer

For Overlay

 Use of FCAW is advisable , However you can use Thin wire SAW with C% less than 0.04 which is available, The 0.6 % is max Ni, More over You have to use Lower carbon. PWHT temp. should not be more than 640C (Of course 410 overlay should be on 309Mol barrier layer )

If you want to have bend test please try with initially small er angle of about 120 degree with 60 formaer dia and later on with 40 former dia Loading should be very slow

 

Regards

 

Hegde P.B.

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent: Thursday, April 16, 2009 8:57 AM
To: materials-welding@googlegroups.com
Subject: [MW:1964] FW: 1963] SS 410 overlay with E 309L MO barrier layer

 

 

 


From: Chandra, Vasanthan (Lagos) [mailto:Vasanthan.Chandra@DeltaAfrik.com]
Sent: Wednesday, April 15, 2009 8:30 PM
To: materials-welding@googlegroups.com
Subject: RE: 1963] SS 410 overlay with E 309L MO barrier layer

 

 

1. How many layers deposited with thickness of each layer including barrier layer?

2. Check for Welding consumable chemistry used for welding (Batch No wise).

3. Max Ni content for SS410 for FCAW Consumable is 0.6%. Hence, depends upon your consumable batch no, the chemistry will be achieved. We can’t get 0.6% Ni because of variation in batch no.

4. ‘’C’’ content. Again it is depends upon the batch used. Check for the same.

5. Bend failure: This is might be due to the formation of sigma phases by heat treatment. Hence, choose consumable with extra low carbon and do screening test.

 

Regards,

vasanth

 

 

 

 

 

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of JASPAL SINGH
Sent: 15 April 2009 07:41
To: Materials & Welding
Subject: [MW:1963] SS 410 overlay with E 309L MO barrier layer

 

 

Dear all

 

I have problem in the overlay of SS 410 on SA 516 Gr  70 with FCAW

process

 

  - I am unable to achieve the carbon % 0.06

  - failure in bend test

  - unable to achieve Ni content of 0.6%

 

As required the barrier layer of E309Lmo which contains high value of

Ni and Cr .

 

Please let me know is it possible to achieve 0.6% Ni in clad layer

with height of 6mm only.

 

how to clear the bend test ? or waiver from client is the only option.

 

Looking for you valuable suggestions.

 

JASPAL SINGH

 

919996624244

 


 


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...