Yes you can weld P8 to P8 with E309  and qualify for SS as per F no , In GTAW F no 6  qualifies for Cs and SS also

 

Hegde P.B

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of BHARAT GOLE
Sent: Friday, April 17, 2009 11:49 AM
To: material welding
Subject: [MW:1971] Re: WELDER QUALIFICATION

 

Mr. Dale Jones
As you said to weld with F5 stainless steel filler material which is needed to weld with matching filler on P8 materials.I would like to add more...i.e. as per QW 423 Alternate Base Materials for welder qualification we can weld P1 materiel also with F5 SS Filler  in order to qualify welder for any particular P8 WPS.
This is economical as well as within limit of code.
Please correct me if my interpretation is wrong
Regards

Bharat B. Gole

 





Date: Thu, 16 Apr 2009 16:26:34 -0700
From: dalejones7978@yahoo.com
Subject: [MW:1970] Re: WELDER QUALIFICATION
To: materials-welding@googlegroups.com

This is correct that the welder can weld on all of these materials but do not ignore the other variables. For example the welder will be restricted to the Fnumber filler material he qualified with. An example is a SMAW qualification. When a welder qualifies on P1 material with a matching F4 SMAW filler he will be qualified to the base material range stated below and with F1-F4 carbon steel filler material. This will not qualify him to weld with F5 stainless steel filler material which is needed to weld with matching filler on P8 materials. The same concept will apply to various other P numberd materials. To fully understand this concept and the other variables that will restrict a welders qualifications, read article 3 and QW-416 in ASME Section 9

Regards,

Dale Jones

--- On Thu, 4/16/09, Muhammed Ibrahim <ibratech@gmail.com> wrote:


From: Muhammed Ibrahim <ibratech@gmail.com>
Subject: [MW:1968] Re: WELDER QUALIFICATION
To: materials-welding@googlegroups.com
Date: Thursday, April 16, 2009, 5:45 AM

 

 

Not only P11. Also P34 & P41 thru P49. The reason is, the skill of the welder required to weld any of these material is same. So he can proove it in any one P No. mentioned .

 

Regards,

Muhammed Ibrahim


 

2009/4/16 gaurav mongia <er.gauravmongia@gmail.com>


IF A WELDER IS QUALIFIED FOR P1 material and in code it is written
that he is qualified upto P11.

i wanna know what will be reason that a welder can do welding on all
material upto P11 instead he is only qualified in P1






 


How fun is this? IMing with Windows Live Messenger just got better.

 


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35693] egwuanimkwujacobisrael@gmail.com

Dear all, No. MPI can only detect defect that is 1 to 2 mm dept. Therefore the paint must have mask the defect. Thanks. Egwuanimkw...