Re: [MW:35656] CONSUMABLE SELECTION P9, P5B, P8 Base metal.

For welding the specified base metals—P9 to P9, P5B to P5B, and P5B to P8 (304H)—the selection of consumables (filler metals) must 

consider the chemical composition, mechanical properties, and service conditions of these materials.

Consumables for Joining P9 to P9

·        P9 corresponds to 9Cr-1Mo steels (Chromium-Molybdenum steels).

·        Recommended filler metals for welding P9 to P9 are typically E80S-B8 or E8016B8/E8018-B8 electrodes for GTAW or corresponding 

       solid wires for SMAW.

·        Preheat and post-weld heat treatment (PWHT) are essential to avoid cracking and ensure weld integrity.

Consumables for Joining P5B to P5B

·        P5B includes 5%Cr, 0.5%Mo often used in high-temperature, creep-resistant applications.

·        Common filler metals include ER80S-B6 or E8016-B6/E8018-B6 low alloy wires, which match the Cr-Mo content and provide good 

       weldability and creep strength.

·        Preheat and post-weld heat treatment (PWHT) is mandatory for P5B welds to achieve crack free weld.

Consumables for Joining P5B to P8 (304H SS)

·        This is a dissimilar metal weld between a Cr-Mo steel (P5B) and an austenitic stainless steel (P8 304H).

·        The filler metal must accommodate differences in thermal expansion and metallurgical compatibility.

·        Nickel-based filler metals such as ERNiCrFe-2 or ERNiCrFe-3 (AWS A5.11 or A5.14 classifications) are preferred for joining these dissimilar 

       because they provide good corrosion resistance and reduce the risk of cracking caused by dilution and thermal mismatch.

·        Austenitic stainless steel fillers like ER309 are not recommended for P5B to P8 welds due to dilution issues and stress concentration. Instead, 

       nickel-based alloys with higher corrosion resistance and ductility are used.

·       This selection ensures metallurgical compatibility, mechanical integrity, and service life of the welds involving these materials. Proper welding 

       procedure and heat treatment are critical, especially for creep-resistant steels like P5B and P9.

 

C Sridhar.

--------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


On Thu, 29 May 2025 at 16:24, Ch Bilal jovinda <chbilaleng1989@gmail.com> wrote:
Hi Dear Experts,
  My query is about the selection of welding consumable for GTAW and SMAW process with following combination of Base metals,
1. P9 to P9  
2. P5B to P5B 
3. P5B to P8 304H 

Regards,
M Bilal
Welding engineer.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAOq7hqsqQg7WzZQnTnjSesbx33zF36B9QOKfmvo_Qr9rKQzv6A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYii4DB-_uxz1JzY8%2BKZuJsKk5YoWo6kCq4--racmqD8b5A%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...