Saturday, October 15, 2022

Re: [MW:33600] FW: 33587] Black dots on sdss welding

Will cleaning the Filler Rod and Joint using a solvent like Acetone will solve this problem.




On Wednesday, 12 October, 2022 at 08:06:31 pm GMT+4, <pgoswami@rogers.com> wrote:


 

Hi Narayanan,

 

Please refer the discussions and the answers provided the following link. The spots may appear due to few issues:

  • Type of lubricants used during wire drawing of the GTAW filler wires. Typically oil based lubricants if used could generate such residues, while soap type lubricants  may not.
  • Surface finish of the SDSS. If the products are acid cleaned & pickled after manufacturing the chances of such welding dross would be less.

Irrespective of those facts, the discussions in this following link are worthwhile to look at.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

Black spots on DSS Weld Joints. (google.com)

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Narayanan Kumar
Sent: October 11, 2022 9:31 AM
To: materials-welding@googlegroups.com
Subject: [MW:33587] Black dots on sdss welding

 

Dear Team,

 

Can you please explain about the black dots appears on SDSS GTAW Weld bead( ER 2594 )  with document backup for the causes 

 

 

Regards,

 

M.Kumar 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADTvyj%2B9Ti77s60HeABOGGgrcOeok0BG2nwCqMQQ8zrDqdyGyw%40mail.gmail.com.


Virus-free.www.avg.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAAD52mhkWpdIT6LX5J7kKqpxAQAAAAA%3D%40rogers.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...