As per 7.8.1, para 2,
rate of heating ia 560/2"= 280Deg.C

But there is a condition that "but in no case more than 220Deg.C per hour.

Hence you have to apply 220 Deg. C per hour. 



On Fri, Oct 7, 2022, 11:13 AM Student <nabeel233@gmail.com> wrote:
Dear All
Please guide how to calculate the rate of heating for PWHT for below AWS d1.1

"Para 7.8.1 Above 600°F [3 1 5 °C] , the rate of heating in °F [°C] per hour shall not exceed 400 [560] divided by the maximum
metal thickness of the thicker part, in inches [centimeters ] , but in no case more than 400°F [220°C] per hour"

If the maximum thickness is 2 inches , how to calculate heating rate

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/007241e8-ef96-424b-b22f-136b00673b26n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPHaPBKC2dE60TrM8VSS1vPM3yutKdrUdYC0eU5PpKdQRGM5SA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...