Re: [MW:30924] SS-316L Rusting

SS welded regions readily rust in the presence of moisture ,unless iron from welding fume deposits are immediately removed.

It is a very common issue and shows a lack of attention to post welding clean-up.

At least wire brushing is the minimum necessary application.

The rusting is the oxidation of the condensed iron on the SS weldment surface and surrounding zone.

D Harvey, PhD.

No comments:

[MW:35668] Selection of Filler/Electrode.