RE: [MW:29635] I need to do dissimilar weld joint (6xxx series Aluminium to Steel). What filler wire should I choose?

Aluminum can't be directly welded to Steel by any Arc welding process. Arc welding between any steel to aluminum causes formation of intermetallic compounds at the interface, which makes the weld joint extremely brittle. Look at the YouTube, there're many videos on this subject.

 

The only way to perform arc welding of such dissimilar combination is to use a transition piece  of steel to Aluminum, produced by solid state welding process.

This article from ESAB , explains some of the problems of such welding.

 

Thanks.

P.Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: 'Karthik' via Materials & Welding [mailto:materials-welding@googlegroups.com]
Sent: May 23, 2019 10:07 PM
To: Materials & Welding <materials-welding@googlegroups.com>
Subject: Re: [MW:29631] I need to do dissimilar weld joint (6xxx series Aluminium to Steel). What filler wire should I choose?

 

Hi,

The attached file might be useful to you.

 

Thanks& Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager

Agon Pacific Co.,Ltd.

M: +66-655-174-397, +66-892-512-282

E-mail : karthik6684@yahoo.com

 

 

On Thursday, May 23, 2019, 6:44:48 PM GMT+7, Ram <rameshsmit@gmail.com> wrote:

 

 

I need to do dissimilar weld joint (6xxx series Aluminium to Steel). What filler wire should I choose?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7206cf51-d3f4-413a-838e-3036e9ad1a26%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1605684784.4306536.1558663626710%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...