Tuesday, September 20, 2016

Re: [MW:25432] Re: Using of ER70S-6 in place of ER70S-2

The A No 1 in the WPSs and PQR with ER70S-6 is a common finding during ASME joint reviews. In such cases just insert a note in the WPS on Mn and Si max content

2016-09-19 3:05 GMT+03:00 John Henning <jhenning@deltak.com>:

Your comment on ER70S-6 is most certainly untrue.  GTAW with ER70S-6 will yield superbly clean welds and exceed all X-ray requirements provided the base metal is clean to start with.  The bonus is that ER70S-6 will have significantly better impacts than ER70S-2 especially when PWHT is required.  In my experience, welders seem to like the flow and wetability characteristics of the -6 over the -2.   The downside of -6 is that as the Mn and Si are higher, it is more difficult to reduce the hardness of the weld.  Also, to meet many petro-chem requirements for A1 chemistry limits for carbon steel filler metals, one often has to specify a maximum of 1.6% Mn and 1.0%Si.  This typically is not a problem for filler metal suppliers.


Triple deoxidized ER70S-2 is often preferred for the first pass of an open root joint.  But the presence of these deoxidizers leads to welds with far more inclusions (microscopic SONIMS) than with -6.  The plethora of SONIMS results in the overall poorer impact performance. 


Enjoy - 


From: 'c sridhar' via Materials & Welding <materials-welding@googlegroups.com>
Sent: Saturday, September 17, 2016 6:10 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:25410] Re: Using of ER70S-6 in place of ER70S-2
 
You have not mentioned the welding process in use at your end

If it is TIG, flat no. as 70 S2 contains triple deoxidisers Al, ZN & Ti and used with argon gas.
ER 70S06 does not have them and will not give x-ray quality welds.

If it is MAG/CO2 process or with argon gas, you can go ahead. 

Ti addition alone with 70 S6 do not help. S6 also contains excessive Mn & Si and not used for 
TIG process.

Sridhar.


From: sanjeev singh <sanjeevsinghfbd@gmail.com>
To: Materials & Welding <materials-welding@googlegroups.com>
Sent: Thursday, 15 September 2016 11:40 AM
Subject: [MW:25396] Re: Using of ER70S-6 in place of ER70S-2

Please guide- If we add Ti in ER70S-6 in range of 0.011%, what will be the effect during CO2 welding?

regards,

Sanjeev

On Thursday, 10 January 2013 12:13:36 UTC+5:30, Ranendra Chakraborty wrote:
Dear Expert,
Please guide whether ER70S-6 can be used in place of ER70S-2. Please give code reference.
 
Regards,
Ranendra
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/07c21334-a631-40b0-b66e-65075cde9914%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/81069408.169321.1474110634168%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/MWHPR03MB281615CF5428E48D9F21CF18A1F50%40MWHPR03MB2816.namprd03.prod.outlook.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CA5w2m6sFNh6%3DR-wEg77tstGp2b1BtaZj6VDarmedoEA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...