Thursday, September 15, 2016

[MW:25399] RE: 25392] PWHT

·         Check the project client specifications to see if PWHT is mandatory. It is unlikely.

·         The international standard pipeline design/installation codes would not require PWHT for a pipeline of this diameter and wall thickness.

·         The main reason why you may need to apply PWHT is to meet the required hardness limit which the client specification will inevitably require. That is to say if you fail to meet the specified maximum hardness during welding procedure qualification then PWHT would be one way of changing that situation, but not the best way for production reasons. Alternatively your welding engineer should know how to manage this issue by other means, avoiding PWHT, for example by applying more preheat, controlling the sequence of weld passes or by increasing the thermal input during welding.

·         The reason for the hardness limit is to avoid sulphide stress corrosion cracking caused by the H2S in the sour condensate. Contrary to what others have said hardness control does not affect hydrogen induced cracking susceptibility, which will occur if the linepipe is susceptible to it and there is H2S in the product. You have to have pipe which has been shown not to be susceptible to HIC.

 

Alan Denney

AKD Materials Consulting Ltd

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of zhy370137@gmail.com
Sent: 14 September 2016 15:59
To: Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:25392] PWHT

 

Dear sir

good day 

pls hlep us confirm whether we need apply PWHT for every girth weld according to your experience.

pipe API 5 L X60 HIC resistant pipe

welding method: CRC automatic

pipeline diameter and thickness:20inch 0.4inch(10MM)

mediumsour condensate 

pressure:960psi

pipeline distance164km between two gas plant in saudi safaniya plant to berris gas plant)

clientsaudi aramco

 

CNPC daqing saudi 

QAQC

 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f49f77aa-d202-4cc2-91c7-b5f1f828afcd%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...