Dear jainul,
for PQR qualification 2 tensile+2 face bend + 2 root bend require
for speciment size you can refer 462.1C for tensile and 462.3B for root and face bend.
regarding imapct requirement since B444 is suitable for use upto -198C and as per B31.3, 323.2.2,A6(a) and A6(b) impact test is not require for temperature you have mentioned -28C to 37C.
hope this help.
regards,
mohd.
On Sunday, November 3, 2013 8:54:26 AM UTC, Jainul Abudeen wrote:
Dear experts,
Please provide mechanical test need to qualify PQR for Inconel material as per specification.
Piping material Specification - ASTM B444 UNS NO6625 GR.I ( CU-NI)
Pipe thickness/schedule - 80 SCH
Pipe Inch - 1"
Design Temp - -20/220 FPlease take advise us as soon as possible.Note : Toughness is required or not?
Regards,
Jain,
QC Engineer
055822475
--
Regards & Thanks,
Jainul Abudeen.A
QA/QC Engineer,
Punj Lloyd Ltd.,
+918861133635
SAVE PAPER - SAVE TREE - Please do not print this e-mail unless necessary.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
Comments