Skip to main content

Re: [MW:12703] CLAD MATERIALS -WELDING

Dear Elumalai,

For inconel clad pipe welding (no access from inside) must be completed with inconel E/ERNiCrMo-3 filler material.

 

CS filler materials shall not directly welded on inconel base/ weld metal in order to avoid dilution which will end up with micro cracks on fusion line. This is due to CS electrodes which is basically without addition of alloying elements, while welding the weld pool tends to pick up more alloying elements from inconel base or weld metal (% of dilution is very high around 60%) which is martensitic structure (susceptible microstructure) and more prone to cracking problem. However, on the other hand if we use inconel filler on CS, the % of dilution will be minimized and the final microstructure at fusion line is not in martensitic and hence it is recommended to use only inconel filler metals. Attached herewith some articles on inconel clad pipe welding and bevel preparation for clad portion of welding.

 

The following alternate filler metals can be proposed and qualified.

 

Option 1: Complete weld with inconel filler (ER/ENiCrMo-3)

Option 2: Root and second pass with ERNiCrMo-3 and rest by ENiCrFe-3

Option 3: Root and second pass with ERNiCrMo-3 and rest by E310 (super austenitic)

 

Your proposal is not acceptable. However, the following can be proposed and qualified with risk.

 

Root and second pass with ERNiCrMo-3 and next pass with pure iron electrodes and rest of the passes with E7018 or any CS electrodes. Till now there is no proven record for this case since control on weld pool and using pure iron electrodes requires high skill and even though it cannot be assured sound weld on all pipe joints.

 

Let me know your feedback.

 
Regards,
 
L. Prabhu kumar.


From: Sundaram Elumalai <Elumalai.Sundaram@starfab.com.sa>
Sent: Mon, 17 Oct 2011 17:23:44
To: <materials-welding@googlegroups.com>
Subject: [MW:12682] CLAD MATERIALS -WELDING

Hi experts,

 

We have the following Clad Pipe and we are preparing WPS /PQR to weld this SPOOL. As I know we need to use ERNiCrMo3 / E NiCrMo 3 ( if GTAW+SMAW) to Complete weld. But if any one is having experience with this, please advice whether we will go with

 

GTAW -  ER NiCrMo3  ( First four Passes- R/H/F1/F2)

SMAW – E7018-1  ( Balance Filling /Capping).

 

We have Pitting corrosion test as per ASTM G48 at 50 degree.

 

Pipe

NPS:10-Thk:45mm-PIPE-API 5L GR.X65 PSL2 - SMLS -GA-E-61036

BW

3mm Inconel Cladded

Pipe

NPS:12-Thk:15.88mm-PIPE-API 5L GR.X65 PSL2 - SMLS -GA-E-61036

BW

3mm Inconel Cladded

Pipe

NPS:12-Thk:45.5mm-PIPE-API 5L GR.X65 PSL2 - SMLS -GA-E-61036

BW

3mm Inconel Cladded

Pipe

NPS:12-Thk:53.5mm-PIPE-API 5L GR.X65 PSL2 - SMLS -GA-E-61036

BW

3mm Inconel Cladded

 

 

 

With Kind Regards,

 

S.Elumalai.

******************************************************************************************
CONFIDENTIALITY NOTICE
This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this e-mail and any attachments permanently from your system.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Follow Rediff Deal ho jaye! to get exciting offers in your city everyday.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...