www.t-put.com/EN_welding_C​rMo.pdf

The above link is a good guideline for welding Cr-Mo steels. In page 3, figure 2 (left) demonstrates a good temperature cycle and heat control during welding and PWHT of martensitic P91 & P92 steel...

Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
   



On Wed, Jul 27, 2011 at 7:13 PM, Izhar Mustafa <izharmustafa@gmail.com> wrote:
Use ER90S-B9/E 9015-B9 welding consumable and use Induction method for pre-heat or Interpass temperature maintenance,,Set minimum 200C temperature and After welding do Intermediate post weld heat treatment. i.e after welding keep temperature minimum 250C and hold it minimum 1hour then cool down by 75C/h then allow free cooling under insulation.

Hope for the best,,,,

Wishes

Izhar.


On Wed, Jul 27, 2011 at 7:14 PM, sudhakar kuppuswamy <mechsudhakar@gmail.com> wrote:


dear all, 
please share your experience in repair welding of P91 or P92 ? please post your valuable welding tips like preheating techniques,filler metals that can be used for repair & so on !!!


With regards,
Sudhakar.k

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...