Re: [MW:11952] Suggest Consumable for AISI 4135 material Reg.,

Dear KCR,
Please follow the following:
GTAW :root & Hot pass :ER 80SB2
SMAW:F& C:E10018D2
Preheat Min 100 Deg C
Max Interpass :250 Deg C
PWHT:Min 610 +/- 10 degree C

This would be fine, but check your thickness & impact requirements.

Regards,
Vg

On Wed, Jul 27, 2011 at 12:36 PM, kcrtechnical <kcrtechnical@gmail.com> wrote:
Dear Friends
please suggest suitable best electorde and filler material for AISI 4135 material and Preheat and PWHT requriements.
 
Best regards
K C R

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...