Friday, May 6, 2011

Re: [MW:10977] heat input calculation

dear Martin,
USE  VI/S TO GET JOULES/MM(VOLTAGE*CURRENT/WELDING SPEED)
71*9.5/3.2*25/60
regards
Dr.K G K MURTI

On Fri, May 6, 2011 at 11:00 AM, Martin Prad <martin_prad@hotmail.com> wrote:
gents,
 
how to calculate the heat input in KJ/mm if i have got the folowing parameters?
 
Amperage=71
Voltage=9.5
Travel speed=3.2 inch/minute
can you please put these in the formula?
 
thanks.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...