[MW:10989] Re: Reg: how to select filler wire for dissimilar metals

Yes, you can use SFA 5.11 E NiCrFe-2 or SFA 5.14 ER NiCr-3 for HK-40
(centrifugal casting alloy) to P9 material welidng.

Cheers!

Raj

On May 4, 2:51 pm, venkat kumar <vssl...@gmail.com> wrote:
> dear experts,
>
> pl guide me that how to select filler wire according to given material.for
> instance if material is dissimilar, base material having 9Cr,1Mo,other
> material SA 351 HK 40,having Cr.23-27,Ni.19-22.one of our expert suggested
> that ErNiCr-3 as a filler wire.Other than material what characteristics are
> we have to take in to consideration to select filler wire.
>
> thanks & regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...