Re: [MW:35931] Black soot in MIG

Dear,

ER70S6 filler wire suitable but the problem is more about surface chemistry of aluminized steel and gas composition than filler wire choice.
My suggestion as below
1) Avoid pure Argon for MIG on steel—it can cause poor penetration and lack of fusion.
2) Change gas mix to 97% Ar / 3% O₂.This stabilizes the arc and reduces oxidation
3) Slightly increase gas flow i.e 14–16 L/min.
4) Use forehand (push) instead of pull to direct fumes away from the weld.

Regards,
Pravin Nimbalkar

On Friday, April 1, 2022 at 5:11:22 PM UTC+5:30 Anthony Dalisay wrote:
I thought of doing the same too, however, it will cost me down time to remove the surface aluminium of all the items (about 40k pieces). You are correct that it is natural tendency for aluminium to oxidize when diffused with the weld arc, although this seems to be illusive, would changing the gas flow rate(to higher), welding progression(from pull to push) and angle of torch and contact tip to work distance (CTWD) will help eliminate the black soot? I have not tried those I mentioned yet except adjusting the CTWD to much closer distance to base material but surely I will try and see if that would work. I you think I missed something out please feel free to mention it.

If this black soot still occurs, I might switch to High Purity Argon as my last resort and see if thats going to be a success. I let you guys know the result of this experiment shortly. I appreciate all your inputs.

Regards,
Anton

On Fri, 1 Apr 2022 at 7:10 PM 'james gerald' via Materials & Welding <material...@googlegroups.com> wrote:
Sorry i mistook it to be aluminium alloy 7065. IN Aluminiumized sheets welded using carbon steel filler you can prevent black spots by removing aluminium  from the steel sheet in the area of welding  and avoid diffusion of Al into weld metal as Al as a naturally tendency to oxidize as Al2O3

Thanks & Regards

J.Gerald Jayakumar




On Friday, 1 April, 2022, 04:25:10 pm IST, Anthony Dalisay <anthony...@gmail.com> wrote:


This is actually for motorcycle industry and the base material is not of any kind of pure aluminium series. It is an aluminized sheet welded by a robotic MIG using a normal carbon steel filler wire. With given parameters in the email thread.

Regards,
Anton

On Fri, 1 Apr 2022 at 6:24 PM 'james gerald' via Materials & Welding <material...@googlegroups.com> wrote:
seems to be like Aluminium alloy with slight additions of Zn, Mg & Cu mostly in Aerospace industries,

Thanks & Regards

J.Gerald Jayakumar



On Friday, 1 April, 2022, 09:26:43 am IST, Anthony Dalisay <anthony...@gmail.com> wrote:


Filler wire is ER70-6S @0.8 diameter size. 

On Fri, 1 Apr 2022 at 11:45 AM Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:
what is welding rod classification

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Thu, Mar 31, 2022 at 3:36 PM 'james gerald' via Materials & Welding <material...@googlegroups.com> wrote:
Try AC current

Thanks & Regards

J.Gerald Jayakumar




On Thursday, 31 March, 2022, 01:03:59 pm IST, Anthony Dalisay <anthony...@gmail.com> wrote:


Dear experts,

We have been welding aluminized sheet using MIG welder with the following parameters:

Amps: 125
Volts: 29.5
TS: 50cm/min
Gas flow rate: 12L/min
Gas type : 18%CO2 and 82%Ar

However, I cant get rid of black soot (smoke) in the weld vicinity. What do you think, is the best way to do to achieve cleaner weld in aluminized sheet such as this? 

Refer to attached photo for reference.



Thanks in advance for your expert advice.

Regards,
Anthony
--
Anthony Dipasupil Dalisay
TWI AWeldI

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALBzUBLiVBU2wnkd3MGhgAMdC%2BMzEjF4SXM%2BsdgMXQgp5MVh9Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1137188882.137058.1648720763794%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePZEcu3VQAqckVb0QXUPyn68MgPEG3szWJQFaSr%3DVKPHA%40mail.gmail.com.
--
Anthony Dipasupil Dalisay
TWI AWeldI

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/813151293.374227.1648808146903%40mail.yahoo.com.
--
Anthony Dipasupil Dalisay
TWI AWeldI

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
--
Anthony Dipasupil Dalisay
TWI AWeldI

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/d523a089-c8d7-42c7-abf2-d16e77163089n%40googlegroups.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...