Re: [MW:35921] Duplex WPS for Super Duplex

As per ASME Section IX, the use of SDSS filler wire is permitted even when impact testing is not specified or required, provided the essential variables are met.

However, beyond the code requirements, from a metallurgical and performance standpoint, DSS and SDSS differ significantly in their ferrite-austenite phase balance requirements. Achieving the correct phase balance is critical and is strongly influenced by welding heat input. SDSS, in particular, has a higher PREN (Pitting Resistance Equivalent Number) requirement compared to DSS.

To achieve the required PREN and phase balance in SDSS weld metal, nitrogen is commonly added to the shielding and backing gas. Nitrogen is a strong austenite stabilizer and also contributes to an increase in PREN, thereby improving corrosion resistance.

If a WPS is qualified for DSS using pure argon as the shielding gas, and it is later proposed to use an argon–nitrogen mixture (for Eg: Ar + 2% N₂) for SDSS welding, this change would require requalification of the PQR. This is because the addition of nitrogen significantly affects weld metal chemistry, phase balance, and mechanical and corrosion properties, making it a metallurgically significant change even if not explicitly listed as an essential variable in all cases.

That said, if the required mechanical properties, corrosion resistance, and phase balance are successfully achieved using the same gas composition qualified for DSS (i.e., pure argon), ASME Section IX permits its use, as long as all applicable essential and supplementary essential variables remain within the qualified range.

On Mon, 15 Dec 2025, 5:29 pm Alex Kumar Antony, <alexkantony@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/ee5dcbf4-b6cb-4421-8338-04e109d45b15n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ90KGR%2BWjiOTHjPf4mNLed34QHj4QP3_KD%2BzfeckX20tFydUA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...